MDI PrepOLYMER

Kākau pōkole:


  • Kumukūʻai FOB:US $ 0.5 - 9,999 /'āpana
  • MIN.TORRES TIMY:100'āpana /'āpana
  • Manaʻo hiki:10000'āpana /'āpana i kēlā me kēia mahina
  • Kahua o ka Mana:Kina
  • Kūʻai:Ino hoi
  • Huahana kikoʻipiop

    Nā Kūlana Huakaʻi

    Paʻakikī: Shore A 75a - Shore A 95a

    ʻO ka huahana nā hiʻohiʻona o nā mea maikaʻi maikaʻi, ke kūleʻa a me nā mea pono maikaʻi loa.

    Ua hoʻohanaʻia no ka hanaʻana i nā huahana'ē aʻe polytomer

     

    Hōʻailona

     

    D5560

    M2575

    D2590

    D3565

    D3575

    D3590

    Nco /%

    6.0 ± 0.2

    7.5 ± 0.2

    9.0 ± 0.2

    6.5 ± 0.2

    7.5 ± 0.2

    9.0 ± 0.2

    Kahi Aupuni i 20 ℃

    ʻO ka'ōnaehana PTMG, keʻokeʻo keʻokeʻo

    ʻO ka'ōnaehana polyester, keʻokeʻo keʻokeʻo

    Bdo100g prepololmer / g

    6.1

    7.8

    9.3

    6.8

    7.8

    9.3

    Hawaiian (85 ℃) / Mpa · S

    1400

    1000

    750

    1400

    1200

    1000

    Ka huiʻana i ka mahana / ℃ (prepollymer / 1,4bd)

    80/40

    80/40

    80/40

    80/40

    80/40

    80/40

    Gel Time / min

    10

    8

    7

    10

    8

    7

    E PA MAKA VUKIN KAHIKI (110 ℃) / H

    48

    48

    48

    48

    48

    48

    Paʻakikī (kahakai a)

    87 ± 2

    90 ± 2

    95 ± 2

    85 ± 2

    90 ± 2

    95 ± 2

    100% modulus / mpa

    6

    9.2

    12.6

    5

    8.6

    12.3

    300% Modulus / MPA

    17

    166

    18.9

    10

    19.7

    29.1

    Ikaika ikaika / mpa

    44

    43

    45

    50

    46

    55

    Elongation /%

    472

    683

    500

    540

    580

    530

    Ka ikaika o ka ikaika / (kn / m)

    75

    110

    130

    82

    117

    132

    Rebound /%

    61

    64

    55

    43

    35

    39

    Density (24 ℃) / (g / cm3)

    1.11

    1.11

    1.12

    1.23

    1.26

    1.24

    Hana lole / mm³

    36

    44

    44

    32

    35

    38