Hardness: Shore A 75A - Shore A 95A
Hilber xwedî taybetmendiyên berxwedana xweş, berxwedan û taybetmendiyên mekanîkî yên xweş e.
Ji bo çêkirina hilberên polyurethane yên elastomer ên wekî çîçikên gomik, plakayên sifir û rûkên sekinandinê hatine bikar anîn.
Cins
| D2560 | D2575 | D2590 | D3565 | D3575 | D3590 |
Nco /% | 6.0 ± 0.2 | 7.5 ± 0.2 | 9.0 ± 0.2 | 6.5 ± 0.2 | 7.5 ± 0.2 | 9.0 ± 0.2 |
Dewleta 20 ℃ | Pergala PTMG, solid spî | Pergala polyester, solid spî | ||||
Bdo100g pêşgir / g | 6.1 | 7.8 | 9.3 | 6.8 | 7.8 | 9.3 |
Viscosity (85 ℃) / MPA · s | 1400 | 1000 | 750 750 | 1400 | 1200 | 1000 |
Germahiya tevlihevkirinê / ℃ (PHEPLOLYMER / 1,4BD) | 80/40 | 80/40 | 80/40 | 80/40 | 80/40 | 80/40 |
Gel Time / Min | 10 | 8 | 7 | 10 | 8 | 7 |
Wexta Vulcanization Post (110 ℃) / h | 48 | 48 | 48 | 48 | 48 | 48 |
Hardness (Shore A) | 87 ± 2 | 90 ± 2 | 95 ± 2 | 85 ± 2 | 90 ± 2 | 95 ± 2 |
100% modulus / mpa | 6 | 9.2 | 12.6 | 5 | 8.6 | 12.3 |
300% modulus / mpa | 17 | 16.6 | 18.9 | 10 | 19.7 | 29.1 |
Hêza Tensile / MPa | 44 | 43 | 45 | 50 | 46 | 55 |
Elongation /% | 472 | 683 | 500 | 540 | 580 | 530 |
Hêza tirşikê / (kn / m) | 75 | 110 | 130 | 82 | 117 | 132 |
Rebound /% | 61 | 64 | 55 | 43 | 35 | 39 |
Dendik (24 ℃) / (g / cm3) | 1.11 | 1.11 | 1.12 | 1.23 | 1.26 | 1.24 |
DIN Wear / MM³ | 36 | 44 | 44 | 32 | 35 | 38 |